During a scheduled maintenance outage at a power plant, routine inspections conducted in accordance with the established inspection plan revealed multiple intermittent cracks in the welds of a Y-shaped forged tee on the turbine-side main steam pipeline. This paper presents the inspection findings and the procedures used to assess and repair the defects. Finite element analysis was also performed to evaluate the stress distribution in the main steam pipe tee, taking into account its operating conditions and structural characteristics. Based on the analysis, the causes of the cracking were identified, and optimization recommendations were proposed in the following areas:
- Tee structural design
- Defective weld repair
- Welding procedures and post-weld heat treatment
The cracking problem was ultimately resolved. The findings provide a useful reference for the inspection and repair of similar forged tees.
Unit 6 is a 200 MW coal-fired steam turbine generator set equipped with an ultra-high-pressure, natural-circulation boiler (Model HG-670/13.7-YM17) manufactured by Harbin Boiler Works Co., Ltd. The boiler features a single-furnace, I-shaped, semi-open layout, an all-steel suspended structure, balanced draft, and four-corner tangential firing. It is designed to burn bituminous coal, with reheat steam temperature controlled by flue gas dampers. The unit was commissioned in August 2006 and has accumulated 102,791.57 operating hours.
The main steam piping extends from both sides of the high-temperature superheater outlet header and converges into a single pipeline at the front of the furnace, at an elevation of 34.5 m. It operates at 13.73 MPa and 540°C and is made of 12Cr1MoVG steel. The main steam tee, located on the second-level turbine floor, is a 45° Y-shaped forged welded tee made of 12Cr1MoV steel, with dimensions of Φ486 mm × 70 mm. The associated piping specifications are as follows:
Main steam pipe run (header) at the tee: Φ426 mm × 45 mm, 12Cr1MoVG steel
Main steam pipe branch connected to the tee: Φ325 mm × 34 mm, 12Cr1MoVG steel
Branch between the large-to-small reducer (FI) and the main steam valve: Φ325 mm × 34 mm, 12Cr1MoVG steel
The main steam pipeline operates under high-temperature and high-pressure conditions. In view of lessons learned from power plant accidents in recent years, particular attention must be paid to the inspection and supervision of large-diameter tee fittings. Accordingly, during the scheduled maintenance outage of Unit 6, a comprehensive inspection was conducted in strict accordance with the applicable regulations. The Y-shaped, 45° forged welded tee ST1 is located above the second-floor platform of the turbine hall. A partial schematic of the main steam piping system containing this tee is shown in Figures 1 and 2.

Figure 1. Partial Schematic of the Main Steam Piping System Showing the Location of Y-Shaped 45° Tee ST1

Figure 2. Schematic of the Connection Between Y-Shaped 45° Forged Welded Tee ST1 and the Inclined Branch Pipe
In accordance with the inspection plan, magnetic particle testing was performed on the external surface of the Y-shaped 45° tee ST1 and its connecting welds. During the inspection, crack indications were detected at three locations along weld H3, which connects the tee to the inclined branch pipe:
Upper section: A crack indication approximately 40 mm long was detected along the fusion line on the inclined branch pipe side (Figure 3).
Lower section: A crack indication approximately 60 mm long was detected along the fusion line on the inclined branch pipe side (Figure 4).
Included-angle region: A crack indication approximately 12 mm long was detected along the fusion line on the tee side (Figure 5).

Figure 3. Crack on the Upper Part of the Main Steam Tee
(a) Crack Location (b) Top View of the Defect Location

Figure 4. Crack on the Lower Part of the Main Steam Tee
(a) Crack Location (b) Bottom View of the Defect Location

Figure 5. Location of the Crack at the Included Angle Between the Main Steam Tee and the Inclined Branch Pipe
A review of the available documentation confirmed that the main steam piping is made of 12Cr1MoVG steel, while the Y-shaped 45° forged welded tee is made of 12Cr1MoV steel. The original welding consumable was E5515-B2-V (trade name: R317). Alloy analysis showed that the chemical compositions of the tested components complied with the requirements of GB/T 5310—2017 (Seamless Steel Pipes for High-Pressure Boilers), GB/T 3077—2015 (Alloy Structural Steels), and GB/T 5118—2012 (Welding Electrodes for Heat-Resistant Steels), as well as the design specifications. The test components and results are presented in Table 1. All measured alloying element contents were within the specified limits.
Thickness measurements were performed on the Y-shaped 45° forged welded tee ST1 and its connecting branch pipes. The measurement locations are shown in Figure 2, where H1, H2, and H3 denote the welds. For the branch pipes, all measurement points were located along the circumference, 50 mm from the corresponding weld. The term "front" refers to the upstream section of the pipe, through which the steam flows first. The measurement points were numbered as follows: Point 1 was located at the top of the horizontal pipe section, with Points 2, 3, and 4 arranged clockwise at 90° intervals in the direction of steam flow. On tee ST1, thickness measurements were taken at the belly and shoulder regions. The measurement results are presented in Table 2, and all measured thicknesses met the design requirements.
Table 1. Chemical Composition of the Tested Components (Mass Fraction, %)
Tested component / Specification | Cr | Mo | Mn | V |
Main steam pipe base metal | 0.96 | 0.30 | 0.50 | 0.22 |
Tee base metal | 0.93 | 0.29 | 0.57 | 0.24 |
Weld H3 connecting the tee to the inclined branch pipe | 0.89 | 0.57 | 0.90 | 0.21 |
GB/T 5310 requirements for 12Cr1MoVG steel | 0.90–1.20 | 0.25–0.35 | 0.40–0.70* | 0.15–0.30 |
GB/T 3077 requirements for 12Cr1MoV steel | 0.90–1.20 | 0.25–0.35 | 0.40–0.70 | 0.15–0.30 |
GB/T 5118 requirements for R317 welding electrodes | 0.85–1.50 | 0.40–0.65 | 0.90 max. | 0.10–0.35 |
Table 2. Wall Thickness Measurement Results for Tee ST1 and the Connected Branch Pipes (mm)
Measurement point | H1, front | H1, rear | H2, rear | Tee ST1 |
−1 | 43.5 | 40.6 | 31.9 | 72.2 |
−2 | 43.9 | 43.2 | 33.0 | 71.8 |
−3 | 44.0 | 43.6 | 32.7 | 73.1 |
−4 | 43.7 | 43.1 | 32.6 | — |
Ultrasonic testing was performed on the Y-shaped 45° forged welded tee ST1 and its connecting butt welds on the main steam pipeline. No unacceptable defects were detected in the tee body. However, three unacceptable defects were identified in butt weld H3, which connects the tee to the inclined branch pipe. Their distribution is shown in Figure 6, and the details are provided in Table 3.

Figure 6. Distribution of Unacceptable Defects in Butt Weld H3 Connecting Tee ST1 to the Inclined Branch Pipe
Table 3. Details of Unacceptable Defects Detected by Ultrasonic Testing
No. | Position | Amplitude (dB) | Depth (mm) | Length (mm) | Acceptance Level | Remarks |
① | 35 mm east of the location shown in Figure 6 | SL+14 | 18–20 | 52 | III | Located along the weld fusion line on the branch pipe side |
② | 10 mm below and west of the location shown in Figure 6 | SL+12 | 11–14 | 59* | III | Located along the weld fusion line on the branch pipe side |
③ | Due east of the location shown in Figure 6 | SL+11 | 9–10 | 12 | III | Located along the weld fusion line on the tee side |
Hardness testing was performed on the body of the Y-shaped 45° forged welded tee ST1 and its connecting butt welds. The test locations are shown in Figure 2, where H1, H2, and H3 denote the welds. The measurement points were numbered as follows: Point 1 was located at the top of the horizontal pipe section, with Points 2, 3, and 4 arranged clockwise at 90° intervals in the direction of steam flow. The test results are presented in Table 4.
Table 4. Hardness Test Results for Tee ST1 and Its Butt Welds (HB)
Measurement point | a | b (H2) | c | d | e (H1) | f | g | h (H3) | i |
−1 | 172 | 205 | 168 | 159 | 209 | 168 | 120 | 215 | 141 |
−2 | 168 | 203 | 157 | 142 | 202 | 171 | 127 | 210 | 148 |
−3 | 159 | 210 | 155 | 144 | 207 | 174 | 131 | 208 | 150 |
−4 | 171 | 203 | 172 | 160 | 213 | 172 | — | 216 | 145 |
The Leeb hardness of the tee body ranged from 120 to 131 HBHLD. According to DL/T 438—2016, Technical Supervision Code for Metal in Fossil Fuel Power Plants, the hardness of 12Cr1MoV steel forgings should be within the range of 118–195 HB. Therefore, the hardness measurements of the tee body met the specified requirements. The hardness of the butt welds connecting the tee to the branch pipes ranged from 209 to 213 HBHLD for H1, 203 to 210 HBHLD for H2, and 208 to 216 HBHLD for H3. According to DL/T 438—2016, the specified hardness range for 12Cr1MoVG steel pipe fittings is 130–197 HB. In addition, DL/T 869—2021, Technical Code for Welding in Fossil Fuel Power Plants, specifies that the upper limit of weld hardness must not exceed the base metal hardness by more than 100 HBW or 270 HB, whichever is lower. The lower limit must be at least 90% of the base metal hardness. Based on these criteria, the hardness measurements of all three butt welds met the applicable requirements.
Metallographic samples were taken from the body of the Y-shaped 45° forged welded tee ST1 and its connecting butt welds on the main steam pipeline. The microstructure in the upper region of the tee body consisted of ferrite and bainite, as shown in Figure 7. According to DL/T 884—2019, Technical Guidelines for Metallographic Examination and Evaluation in Fossil Fuel Power Plants, the microstructure exhibited slight traces of bainitic regions, with noticeable carbide agglomeration and coarsening. Most of the carbides were distributed in granular form along and near the grain boundaries. The microstructural aging was rated as Level 4.

Figure 7. Microstructure in the Upper Region of the Main Steam Pipeline Y-Shaped 45° Tee ST1
A cold-state stress inspection was performed on the supports and hangers around the Y-shaped 45° tee ST1 on the main steam pipeline, including those associated with the adjacent main steam header and branch pipes. No abnormalities were identified.
The test results indicate that the chemical compositions of the Y-shaped 45° tee ST1 and its associated components met the applicable standard requirements. The supports and hangers in the surrounding piping system were in normal condition. The hardness measurements of the tee body and connecting butt welds also met the specified requirements. However, metallographic examination revealed microstructural aging in the tee body. The tee had been in high-temperature service for more than 16 years, with over 100,000 operating hours. Some degree of microstructural aging had therefore occurred, which is considered a normal aging phenomenon under long-term high-temperature service conditions.
Magnetic particle and ultrasonic testing revealed that the crack in weld H3 had measurable length and depth. Its location and morphology indicated that it propagated along the fusion line of the weld connecting the tee to the branch pipe. However, no obvious chamfer had been provided in this area during manufacturing, creating a potential stress concentration that could accelerate crack initiation and propagation. Preliminary analysis suggests that the crack may have resulted from the substantial wall thickness difference between tee ST1 (Ø486 mm × 70 mm) and the connected main steam branch pipe (Ø324 mm × 34 mm). The weld and the tee groove formed a sharp angle, resulting in stress concentration along the weld fusion line on the branch pipe side.
Finite element analysis (FEA) was performed on the tee based on its operating conditions and structural characteristics. A sequentially coupled analysis approach was adopted. First, the temperature field was calculated. The analysis was then switched to structural analysis, with the calculated temperature field applied to the element nodes to determine the resulting stress and strain. The Y-shaped tee was discretized into a finite element model consisting of a finite number of elements and nodes. For the thermal analysis, the model was meshed using the 8-node three-dimensional thermal solid element SOLID70. For the structural analysis, these elements were converted into the corresponding 8-node three-dimensional structural solid elements, SOLID185. The finite element mesh is shown in Figure 8. The physical and mechanical properties of the material used for the Y-shaped 45° forged welded tee are listed in Table 5.

Figure 8. Finite Element Mesh of the Y-Shaped Tee
Table 5. Selected Physical Properties of 12Cr1MoV Steel
Temperature (°C) | Elastic modulus (GPa) | Thermal conductivity [W/(m·K)] | Linear expansion coefficient (×10⁻⁶/°C) | Specific heat capacity [J/(kg·K)] | Allowable stress (MPa) |
500 | 179 | 32.2 | 14.15 | 682 | 113 |
540 | 174.2 | 31.56 | 14.242 | 700.8 | 77 |
600 | 167 | 30.6 | 14.38 | 729 | — |
Note: The physical property values of 12Cr1MoV steel at 540 °C were obtained by interpolation.
Analysis of the crack location and morphology indicates that the crack propagated along the intersection line between the tee and the branch pipe. However, no smooth transition was provided at this location during manufacturing, creating a potential stress concentration that could accelerate crack initiation and propagation. The finite element analysis showed that peak stresses occurred at the roots on both sides of the tee-to-branch-pipe connection, with a higher stress level on the inner side. The direction of the maximum principal stress was consistent with the observed crack propagation direction, as shown in Figure 9.

Figure 9 Stress analysis results
Without a chamfer, the peak stress at this location under operating conditions reached 109 MPa, significantly exceeding the allowable stress of 12Cr1MoV steel at 540 °C (77 MPa). Inspection indicated that the crack initiated at the inner surface and propagated outward toward the outer wall under stress, consistent with the finite element analysis results. Stress analyses were also performed for different chamfer configurations, as shown in Figure 10. The peak stress decreased progressively as the chamfer radius increased. At a chamfer radius of R = 60 mm, the peak stress decreased to 56 MPa, below the allowable stress of 12Cr1MoV steel under operating conditions. This configuration therefore satisfied the material strength requirements without adversely affecting the stress condition of the piping system.

Figure 10 Variation in Peak Stress with Chamfer Radius
The above analysis indicates that the cracks at the roots on both sides of the 45° branch connection of the Y-shaped tee were primarily caused by stress concentration resulting from the tee geometry. Under normal operating conditions, the combined stresses exceeded the allowable stress of the material. The cracks were therefore primarily associated with structural stress concentration rather than material degradation.
Based on the inspection results for the Y-shaped 45° tee ST1 on the main steam pipeline and the analysis of the crack causes, no abnormal material aging or deterioration was identified, and the tee was considered suitable for weld repair. Before welding, the cracks were removed by grinding. The original weld heat-affected zones (HAZs) at the defect locations were completely removed until a clean metallic surface was exposed. Magnetic particle testing was performed during grinding to verify that all cracks had been completely removed.
The dimensions of the excavated areas were as follows:
Lower part of the weld circumference: The crack was 200 mm long, and the maximum excavation depth was 15 mm from the pipe base metal surface.
Upper part of the weld circumference: The crack was 250 mm long, and the maximum excavation depth was 22 mm from the pipe base metal surface.
The ground areas after crack removal are shown in Figure 11.

Figure 11. Tee After Crack Removal by Grinding
Considering the site conditions and structural characteristics of the main steam tee, homogeneous hot welding was adopted to ensure weld quality and support the long-term safe and reliable operation of the equipment. The welding procedure was developed in accordance with DL/T 869—2021, Technical Code for Welding in Thermal Power Plants, and DL/T 819—2019, Technical Code for Welding Heat Treatment in Thermal Power Plants. Gas tungsten arc welding (GTAW) was used for the root pass, while shielded metal arc welding (SMAW) was used for the filling and cap passes. The welding consumables were as follows:
- GTAW wire: TIG-R31, Ø2.5 mm
- SMAW electrode: E5515-B2-V (R317), Ø3.2 mm
Homogeneous hot welding helps maintain the ductility and toughness of the weld metal, provides a good weld bead appearance, and offers good all-position welding performance. However, the large wall thickness and complex geometry of the tee present risks of cold cracking and reheat cracking during repair. Therefore, welding temperatures must be carefully controlled throughout the process. The repair procedure requires:
- Preheating before welding
- Strict control of the interpass temperature during welding
The key welding process control measures are as follows:
Welder qualifications and welding parameters: Welders must hold the appropriate qualifications. The ZX7-400STG inverter welding machine is recommended. Multi-layer, multi-pass welding shall be employed, with GTAW using direct current straight polarity (DCSP) for the root pass and SMAW using direct current reverse polarity (DCRP) for the filling and cap passes. Before welding, the wire shall be cleaned of rust, scale, oil, and other contaminants until a metallic luster is obtained. Electrodes shall be baked in accordance with the specified requirements before use, with no more than two rebaking cycles. The GTAW root-pass current shall be 90–110 A, and the SMAW current shall be 120–140 A.
Crack removal and surface preparation: Any cracks detected in the tee shall be removed by mechanical grinding, followed by magnetic particle testing (MT) to verify complete removal. The weld groove surface and adjacent areas extending 60 mm on each side shall be cleaned of oil, paint, scale, and rust until a metallic luster is exposed.
Preheating and interpass temperature control: Flexible ceramic resistance heating pads shall be used for preheating and installed 20–30 mm from the edge of the weld groove. The temperature shall be monitored and controlled using a computerized temperature control cabinet, with heat transferred from the ceramic pads by radiation. The heating width shall be at least 360 mm on each side of the weld. The preheating and interpass temperatures shall both be maintained at 200–300 °C, with a heating rate of 89 °C/h. The tee weld shall be tightly wrapped with electrolytic asbestos cloth, with aluminum silicate insulation wool used as the external insulation layer. The heat treatment process curve is shown in Figure 12.

Figure 12 Heat Treatment Process Curve
Control of welding technique: During welding, heat input should be kept as low as practicable to prevent overheating and excessive grain growth in the weld metal and thereby improve its mechanical properties. High welding currents and low travel speeds should be avoided. Particular attention shall be paid to joint quality and arc termination. The weld pool must be filled before the arc is extinguished. Repeated arc striking at the same location is strictly prohibited, and the start and stop positions of adjacent weld beads in multi-layer, multi-pass welding shall be staggered.
Welder self-inspection: After completing each weld pass, the welder shall perform a self-inspection. The weld surface shall be free of undercut, porosity, slag inclusions, and cracks. Transitions between adjacent weld beads shall be smooth and free of deep grooves.
Post-weld heat treatment: Immediately after welding, high-temperature tempering shall be performed using medium-frequency induction heating equipment. The heat treatment temperature shall be 730 °C, with heating and cooling rates of 89 °C/h. The temperature shall be held at 730 °C for 2 h. The heating equipment shall be switched off when the temperature reaches 300 °C, after which the component shall be allowed to cool naturally. The heated zone shall extend at least 350 mm on each side of the weld, and the thermal insulation layer shall be at least 490 mm thick on each side.
Post-repair inspection: After the component has cooled naturally to room temperature, the repaired area shall be mechanically ground to ensure a smooth transition between the weld and the base metal. Magnetic particle testing (MT) shall be performed 24 h after heat treatment. The results shall comply with NB/T 47013.4—2015, Non-destructive Testing of Pressure Equipment—Part 4: Magnetic Particle Testing, and meet the Level I acceptance criteria.
After repair welding of butt weld H3 on the main steam tee, the weld surface was ground flush. At the crack locations at the roots on both sides of the 45° inclined main steam branch pipe, the repaired areas were manually ground to form smooth transitions with a chamfer radius of 60 mm, thereby reducing stress concentration.
- Visual inspection: A 100% visual inspection was performed on the repaired welds. No surface defects, such as porosity, pits, slag inclusions, or cracks, were observed. The weld edges exhibited smooth transitions, and the weld dimensions complied with the design specifications and applicable regulatory requirements.
- Nondestructive testing: Following heat treatment, 100% magnetic particle testing (MT) and ultrasonic testing (UT) were performed on the tee body and its welds. No unacceptable defects were detected.
- Hardness testing: Hardness testing was performed on the tee base metal, yielding values of 125–136 HBHLD. The hardness of butt weld H3 ranged from 214 to 228 HBHLD. All results met the applicable standard requirements.
Comprehensive inspection of the main steam tee and its connecting butt welds at the power plant revealed multiple cracks. Root cause analysis confirmed that the cracks were not attributable to abnormal material degradation but were primarily caused by structural stress concentration. A targeted weld repair plan was developed and implemented in strict accordance with the approved welding procedure. In addition, finite element analysis (FEA) was performed to evaluate the tee structure, and the chamfer geometry was optimized to reduce stress concentration.
Although the weld repair and the addition of chamfers have addressed the tee's structural deficiencies and helped extend its service life, the component has already been in service for an extended period. Enhanced monitoring is therefore necessary to ensure its continued safe operation. The following recommendations are proposed:
- Strengthen in-service monitoring: Strengthen integrity monitoring of the main steam tee and its associated welds, and conduct follow-up inspections during scheduled maintenance outages. Where feasible, replace the existing forged-and-welded tee with a one-piece forged tee to eliminate potential equipment risks.
- Improve design review and structural optimization: During project design, strengthen the review of design documents for tees and connected piping to ensure compliance with applicable codes and regulations. Avoid structurally unfavorable configurations, such as directly butt-welding a tee to an elbow, and optimize tee geometry to minimize stress concentration.
- Strengthen manufacturing quality control: During equipment manufacturing, ensure rigorous quality supervision and acceptance inspection of large-diameter tees. Key inspection items shall include alloying element content, hardness, and wall thickness. If any abnormal hardness readings are detected, metallographic examination shall be performed. Where practicable, the transition pipes connected to the tee branches should be welded at the manufacturing facility or piping fabrication shop, and the entire assembly should undergo heat treatment. This helps avoid the risks associated with uncontrolled localized heat treatment during on-site installation.
- Enhance maintenance inspections: During maintenance outages, conduct comprehensive inspections of large-diameter tees, with particular attention to hardness, wall thickness, external surface condition, and welded joints.
- Maintain support and hanger integrity: Regularly monitor the condition of the piping system's supports and hangers and ensure that they are inspected and adjusted as necessary. This helps prevent load loss or overloading, which could upset the load balance within the piping system.
- Ensure proper operating practices: During operation, strictly follow the prescribed operating procedures and control the rates of temperature change and pressure fluctuation to prevent thermal shock and reduce the risk of accelerated degradation of high-temperature components.